Technical
Product Data Sheets
Nylon
6/6
Nylon
6/6 GF-30 (30% glass-fiber
reinforced)
All
NYLON 6/6 materials have high
mechanical strength and superior
resistance to wear and organic
chemicals. NYLON 6/6 GF30 has
more than double the strength and
stiffness of unreinforced nylons and
a heat deflection temperature which
approaches its melting point.
NYLON 6/6 is a 30%
glass-fiber-reinforced nylon 6/6
material whose important properties
include high tensile and flexural
strength, stiffness, excellent heat
deflection temperature, and superior
abrasion and wear resistance.
Typical
Values
| Physical
Properties |
ASTM
Test Method |
Units |
Nylon
6/6 |
Nylon
6/6 GF30 |
| Density |
D792 |
lbs/cu
in |
0.0412 |
0.0488 |
| Specific
Gravity |
D792 |
---- |
1.14 |
1.35 |
| Water
absorption, 24 hours, 73°F
(23°C) |
D570 |
% |
8.5 |
0.7 |
| Mechanical
Properties |
ASTM
Test Method |
Units |
Nylon
6/6 |
Nylon
6/6 GF30 |
| Tensile
Strength 73°F |
D638 |
psi |
12,400 |
27,000 |
| Elongation
73° F |
D638 |
% |
90 |
3 |
| Flexural
Strength, 73° F |
D790 |
psi |
17,000 |
39,100 |
| Flexural
Modulus, 73°F |
D790 |
psi |
4.1
X 105 |
12
X 105 |
| Izod
Impact Strength, Notched, 73°F |
D256 |
---- |
R120
- M79 |
M101 |
| Rockwell
Hardness |
D785 |
ft-lbs/in. |
1.2 |
2.1 |
| Thermal
Properties |
ASTM
Test Method |
Units |
Nylon
6/6 |
Nylon
6/6 GF30 |
Heat
Deflection
66
psi
264
psi |
D648
D648 |
degrees
F
degrees
F |
455
194 |
490
482 |
Max.Temperature
Long Term
Short
Term |
---- |
degrees
F
degrees
F |
170
355 |
230
465 |
| Coefficient
of Linear Thermal Expansion |
see
below |
|
|
|
-20
to -200° F
200
to 460° F |
D696
D696 |
in./in./degrees
F
---- |
4.5
X 10-5
5.0
X 10-5 |
1.2
X 105
---- |
| Electrical
Properties |
ASTM
Test Method |
Units |
Nylon
6/6 |
Nylon
6/6 GF30 |
| Volume
Resistivity, 73°F |
D257 |
ohm-cm |
1015 |
1015 |
| Dielectric
Constant, 60 Hz, 73°F, 50%
RH |
D150 |
---- |
4.0 |
---- |
| Dielectric
Strength |
D149 |
V/mil |
600 |
530 |
|
Plastic Products, Inc. Plastic materials, machining, molding, fabrication |